In the process of plastic PIPE production line, because the operators are not skilled in the process and machine operation, the outer surface of the plastic pipe is often rough, the inner vibrating ring appears, the wall thickness is uneven, and the roundness is not enough. Therefore, it is necessary to adjust the process in time and eliminate the failure of the plastic pipe production line in order to improve the product quality. 

1. The outer surface of the plastic pipe is rough
Adjust the process temperature; reduce the cooling water temperature, the suitable cooling water temperature of the PE pipe is 20-25 °C; check the water channel for blockage or insufficient water pressure; check whether the heating ring such as the barrel and the head is damaged; adjust the water inlet of the sizing sleeve flow; check the performance and batch number of the raw materials; check the temperature of the core of the mold, if it is higher than the temperature of the die section, reduce the temperature of the core; clean the aggregate of the mold;

2. Grooves appear on the outer surface of the plastic pipe
Adjust the water pressure of the sizing sleeve, and the water output should be balanced; adjust the angle of the nozzle in the vacuum setting box to make the pipe cool evenly; check whether there are sundries, burrs, etc. in the die, sizing sleeve, cutting machine and other hardware;

3. Grooves appear on the inner surface
Check whether the inner tube is filled with water. If water enters, pinch the tube blank that has just exited the mold to seal the inner cavity; reduce the temperature inside the mold; clean and polish the mold;

4. A jitter ring appears inside the pipeline
Adjust the water outlet of the sizing sleeve to make it even; adjust the vacuum degree of the second chamber so that the vacuum degree of the rear chamber is slightly higher than that of the front chamber; check whether the vacuum gasket is too tight; check whether the tractor has jitter; Whether the material is uniform;

5. No vacuum
Check whether the water inlet of the vacuum pump is blocked, if it is blocked, clear it; check whether the vacuum pump is working normally; check whether the vacuum pipeline is leaking; check whether the small hole in the middle of the compression screw of the core mold is blocked, if it is blocked, use a thin wire to clear it;
< br> 6. The outer diameter of the pipe is out of tolerance
Adjust the size of vacuum to change the size of the outer circle; adjust the traction speed to change the size of the outer circle; correct the size of the inner hole of the sizing sleeve;

7. The roundness of the pipe is out of tolerance
Adjust the angle of the nozzles in the vacuum setting machine and the spray box to cool the pipes evenly; check the water level in the vacuum setting machine and the spray box, and the pressure of the water pressure gauge to make the spray volume large and powerful; check the vacuum setting machine and the spray box If the water temperature is greater than 35°C, it is necessary to configure a chilled water system or add a spray cooling box; check the water circuit, clean the filter; adjust the process; check and correct the inner hole circularity of the sizing sleeve; Ovality of the pipe;

8. The wall thickness of the pipe is uneven
Adjust the wall thickness on the mold; adjust the angle of the nozzles in the vacuum setting machine and the spray box to make the pipe cool evenly; adjust the water outlet of the sizing sleeve to make the water outlet evenly; disassemble the mold, check whether the screws inside the mold are loose, and re-tighten them; 

9. The plasticizing temperature is too high
Adjust the heating temperature of the mold core, and ventilate and cool the inside of the mold;

10. The cutting length is not accurate
Check whether the length-measuring wheel is pressed tightly; check whether the length-measuring wheel swings, and tighten the fixing bolts of the length-measuring wheel frame; check whether the travel switch of the cutting machine is damaged; check whether the rotary encoder is damaged; Whether the contact of the plug socket is good); each stand-alone shell (PE terminal) should lead the grounding wire to a general grounding point for reliable grounding, and the grounding point should have a grounding stake that meets the electrical grounding requirements, and each stand-alone shell (PE terminal) is not allowed. Connect to ground after series connection, otherwise interference pulses will be introduced, resulting in inaccurate cutting length.

The above is the Common problems and solutions of PE pipe extrusion production line we have listed for you. You can submit the following form to obtain more industry information we provide for you.

You can visit our website or contact us, and we will provide the latest consultation and solutions

Share to:

Send Inquiry

Home> Industry Information> Common problems and solutions of PE pipe extrusion production line
Related Products List

Home

Product

Phone

About Us

Inquiry

We will contact you immediately

Fill in more information so that we can get in touch with you faster

Privacy statement: Your privacy is very important to Us. Our company promises not to disclose your personal information to any external company with out your explicit permission.

Send